33% Glass Reinforced, Nylon 6/6

Processing Considerations for 33% Glass Reinforced, Nylon 6/6

Recommended Processing Considerations: 33% Glass Reinforced, Nylon 6/6

Drying Temperature
180°F (82°C)
Drying Time2-4 hrs. max.
Maximum Moisture0.20%
Rear
480-540°F  (249-282°C)
Middle
520-560°F (271-293°C)
Front
520-560°F (271-293°C)
Nozzel
520-560°F (271-293°C)
Melt Temperature
520-540°F (271-282)°C)
Mold Temperature
80-160°F (27-71°C)
Back Pressure
50 to 100 psi psi

Nylene does not guarantee the accuracy of this information or the suitability of this product for any given application or usage situation.  These values are based on test specimens and should not be used to establish specification limits or fabricate tooling.